您好,欢迎访问三七文档
ASTMF2179-024.1Annealing4.2ThermalShockJan.14,2010FrankCaoForthebenefitofbusinessandpeopleBureauVeritasConsumerProductsServicesShanghaiCoursecode:2ANotestoTrainees受訓者注意1TrainingPurpose培訓目的2TestProcedures测试SUMMARY3NotestoTrainees受訓者注意A4BureauVeritasConsumerProductsServicesDisclaimer聲明•ThisPowerpointpresentationisintendedforyourexclusiveuse.•此文稿陳述之內容為非公開用途。•Anycopyingorreplicationofthisreporttoofforanyotherpersonorentity,oruseofournameortrademark,ispermittedonlywithourwrittenpermission.•所有複印或副本用於其他人或實體,或本名稱或商標需要得到書面許可。•PleasecompletealltheexercisesandreturntoTrainingteamforevaluationwithinaweekaftercompletionofthistraining.•請於完成此培訓後、一星內完成所有練習並交回培訓組作進一步之評價。•ItisapartofevaluationofAnnualAppraisalPerformanceReview.•此評價會作為每年度的工作表演評價之其中一項評審。ANotetoTrainees受訓者注意5TrainingPurpose培訓目的16BureauVeritasConsumerProductsServicesTodeveloptheknowledgeandskillrequiredtoconductannealingandthermalshocktestperASTMF2179-024.1&4.2TrainingPurpose培訓目的17ASTMF2179-02Standardspecificationforannealedsoda-lime-silicateglasscontainersthatareproducedforuseascandlecontainers181.Scope2.Apparatus3.Procedures29Scope110BureauVeritasConsumerProductsServicesScopeThisStandardcoverstheminimumrequirementsforannealedsoda-lime-silicateglasscontainerswhichusedascandleScope111Apparatus212BureauVeritasConsumerProductsServicesApparatus1ApparatusColdwaterbathHotwaterbathBasketTongsTungstencarbidescribe50gritemerypaperTimerRuler13TestProcedures314BureauVeritasConsumerProductsServicesClause4.1Annealing(CPSD-HL-09404-MTHD)退火TestMethodA:tungstencarbidescratchtest1.Scorearoundtheinsideknuckleofthesampleusingthetungstencarbidescribe(applyjustenoughforcesothattheglasssurfaceispenetrated)2.Scorean“X”acrossthesample’sentireinsidebottomsurfaceProcedures115BureauVeritasConsumerProductsServices3.Fillthesamplewithtapwateruptotherimofthesampleorapproximately1infromtheinsidebottomsurfacewhicheveristheminimum,watertemperature:18-25ºC4.Leavethesamplefilledwithtapwaterfor15minto18min5.Afterthetimeduration,pouroutthewaterandexaminethesampleforanyfractures,recordthefindingandnotethetimewhenfailureoccursProcedures216BureauVeritasConsumerProductsServicesTestMethodB:50gritemerypapertest1.Witha50gritemerypaperabradetheentireinnersurfaceofthesample2.Applyenoughpressurewiththeemerypapertopenetratetheglasssurface,ensureallsharpcorners、dimples、indentationsontheinsidesurfaceofthesampleareabraded3.Fillthesamplewithtapwatertoasufficientheighttoallowforacompleteimmersionoftheabradedsection4.Leavethesamplefilledwithtapwaterfor15minto18min5.Afterthetimeduration,pouroutthewaterandexaminethesampleforanyfractures,recordthefindingandnotethetimewhenfailureoccursProcedures317BureauVeritasConsumerProductsServicesNote1.Allsamplewithabottombaseandaneasilyidentifiableinsideknuckle—MethodA2.Ifthesamplehasnobottombasebutaclearlydefinedknuckle—MethodAwithappropriatelysizedwatercontainer3.Forhavebottombasesbutwhichthicknessoflessthan1/8in—methodB4.Ifthesamplehasnobottombaseandaclearlydefinedknuckleanditswallsthicknessoflessthan1/8in---MethodBwithappropriatelysizedwatercontainer5.Ifthesamplehasnobottombaseandnoclearlydefinedknuckle---MethodBwithappropriatelysizedwatercontainer6.Ifthesamplehasnoclearknuckle---methodB7.Ifthesampleisopenendedwithnobottombase---MethodBwithappropriatelysizedwatercontainer8.Forsmallopeningsthatdonotallowforsafescoringoftheinsideknuckleorsurfaceofthebottombythetungstencarbidescribe---MethodBbutapplytotheoutsideofthesampleandsubmergeinwaterProcedures418BureauVeritasConsumerProductsServicesClause4.2ThermalShock(ASTMC149)热冲击1.Determinethecold-waterbathtemperaturebasedontheavailabletapwatertemperature(21±1.11°C),andadjustthetemperatureofthehotwaterbathtobe90degreesF(50°C)higherthanthecoldwater.2.Oncethetemperatureofthehotwaterbathhasbeenestablished,placethesamplesinthehotwaterbathfor5minutes(±10S).3.Removethesamplesfromthehotwaterbathandplacethemintothecold-waterbathwithin15seconds(±1S).Besuretoemptythehotwateroutofthesamplecontainers4.Maintainthesamplesinthecold-waterbathfor30seconds5.Drythecontainersandvisuallyinspectforcrackingorfractures.Reportfindings.Anycrackingorfracturesisconsideredafailure.Procedures519Assignment功課C20BureauVeritasConsumerProductsServices受訓之員功課指引(Instructiontotrainees):•做1份protocol(必需包括需要用以上提及之測試)•做完測試後,記錄所使用有關的測試結果,並複印一份所做的protocol的測試部份及最終報告,作為功課交給組長或有關領導作評核.•Trainingteam將會以protocol最後的報告之結果及組長或有關領導之評語作功課評核.有關組長或領導指引(InstructiontoSupervisor):•監察受訓之員工使用儀器時的手勢及方法是否正確(如應用)•如果是分包頂目,協助受訓之員工進行分包過情(如應用)•有否出現因不當使用而危險動作/情況(如應用)•有需要時協助/敎導受訓之員工•於受訓之員工的功課上作評核,檢查是否有正確填寫測試結果及記錄做測試時的錯誤地方.Assignment功課C21BureauVeritasConsumerProductsServices受訓之員工功課指引(Instructiontotrainees):•AlltheIcebreakerexercisesmustcheckedbyyourimmediatelySupervisororManagerandsendbacktoTrainingDepartmentwithinaweekafterthecompletionoftheclassforfurtherevaluation•所有思维練習必須以英文完成和組長或領導評核,並在此培訓完成後一個星期以電郵方式交到培訓組作評核.有關組長或領導指引(InstructiontoSupervisor):•Provideyourassistanceandadvisewhenneeded•有需要時協助/敎導受訓之員工•CheckalltheIcebreakerexercisesbeforesubmittoTrainingDepartment.•於受訓之員工的思维練習上作評核,檢查是否正確
本文标题:ASTM-F2179-02-Annealed-SLS-Glass-candle-container
链接地址:https://www.777doc.com/doc-6260032 .html