您好,欢迎访问三七文档
德国工业标准DIN标准号标准名称牌号材料号脱氧方式化学成分%不大于下列厚度(mm)的屈服点值ReH,Mpa不小于下列厚度(mm)的抗拉强度,MPa下列取向、厚度、标距下的伸长率值,%不小于下列厚度(mm)的弯心直径(弯曲180°),直径/厚度不同厚度(mm)的冲击功值,J取向L0=80mmL0=5.65热处理温度℃厚度厚度(mm)CPSN≤16>16~40>40~63>63~80>80~100<33~1000.5~<11~<1.51.5~<22~<2.52.5~33~40>40~63>63~100<33~63>63~100>10~63>63~100DIN17100(1980)一般结St331.0035任选----185175310~540≥290纵横1081191210131114121816----2.5333.5--UST37-21.0037任选≤16>16~1000.17(0.21)0.20(0.25)0.050(0.065)0.050(0.065)0.007(0.010)235225215205195360~510340~470纵17181920212625240.51121.52.5U或N+20厚度>10~16时为27-Ust37-21.0036U0.007(0.009构钢质量规范)横1516171819242322.5JRSt37-21.0038R≤40>40~1000.17(0.19)0.20(0.25)0.050(0.065)0.050(0.065)0.009(0.010)235225215215215U或N+2027-St37-21.0116RR≤1000.17(0.19)0.040(0.050)0.040(0.050)-0.5111.51.52U02723N-20St44-21.0044R≤40>40~1000.21(0.24)0.22(0.25)0.050(0.060)0.050(0.060)0.009(0.010)275265255245235430~580410~540纵横1412151316141715181622202119201822.52.5333.5U或N+202723St44-31.0144RR≤1000.20(0.23)0.040(0.050)0.040(0.050)-U02723N-20St52-31.0570RR≤30>30~1000.20(0.22)0.22(0.24)0.040(0.050)0.040(0.050)-355345335325315510~680490~630纵横1412151316141715181622202119201822.52.5333.5U02723N-20St50-21.0050R--0.050(0.060)0.050(0.060)0.009(0.010)295285275265255490~660470~610纵横12101311141215131614201819171816--St60-21.0060R--0.050(0.060)0.050(0.060)0.009(0.010)335325315305295590~770570~710纵横86971081191210161415131412--St70-21.0070R--0.050(0.060)0.050(0.060)0.009(0.010)365355345335325690~900670~830纵横4354657687111010998--备注:1.钢牌号后的数字表示质量等级,相对等级2而言,等级3的钢必须满足脆性断裂不敏感性的较高要求,它表现在冲击韧性试验温度上。2.脱氧方式符号含义为:U-沸腾钢;R-镇静钢(包括半镇静钢);RR-特殊镇静钢,即加入脱氧剂不仅要固定氧还要固定氮(例如Alt≥0.02%)。3.本标准适用于以一般结构钢制造的,在热轧状态或正火状态下供货的型材、棒材、线材、钢板等、本表所列以钢板产品为对象。4.热处理符号含义为:U-不处理;N-正火状态(包括正火轧制)。5.本标准还包括有特殊使用性能的钢产品,它们以在钢牌号St前冠以下列字母表示:Q:具卷弯性能(包括冷弯成形、冷凸缘及及冷卷边);Z:拉拔;P:锻压;K:轧制成型;Ro:焊管。6.冶炼方法由制造厂选择,如用户有要求必须向制造厂提出。7.化学成分:①化学成分括号内的数字是成品分析允许值。②对St52-3,熔炼分析:Si≤0.55%,Mn≤1.60%;成品分析:Si≤0.60%,Mn≤1.7%。③N允许超过表列值,N每增大0.001%,P应比表列值低0.005%。N熔炼分析值最大不得超过0.012%。8.钢板通常的供货状态见下表德国工业标准DIN标准号及标准名称牌号材料号化学成分(熔炼分析)%产品厚度mm正火状态下的力学性能软化退火状态(G)布氏硬度不大于端淬试验淬火温度℃软化退火温度℃正火处理℃淬火温度回火温度℃备注CSi不大于MnP不大于S屈服点RRO.2不小于抗拉强度MPa最小伸长率,%L0=5.65水淬℃油淬℃纵向横向MPaC221.04020.17~0.240.400.30~0.600.045≤0.045≤100230400~5502725156-650~700880~910860~890-540~6801.调质钢是指其化学成分适用于淬硬、在调质状态下具规定的强度同时有良好韧性。表中仅列出非合金钢,本标准还有28个合金钢,详见标准正文。2.牌号中k:含P、S较低的非合金优质钢m:含S带上下限的非合金优质钢。3.冶炼方法由制造厂选择。4.钢必须是镇静钢(不得为半镇静钢)。5.钢板的供货状态可以是:不处理;Ck221.11510.035≤0.03Cm221.11490.0350.020~0.035C251.04060.22~0.290.400.40~0.700.045≤0.045≤16260420~5702523156-880~910860~890-Ck251.11580.035≤0.03Cm251.11630.0350.020~0.035>16~100240420~5702523C301.05280.27~0.340.400.50~0.800.045≤0.045≤16280450~6302321170-870~900850~880-Ck301.11780.035≤0.03Cm301.11790.0350.020~0.035>16~100250450~6302321C351.05010.32~0.390.400.50~0.800.045≤0.045≤16300480~6702119183870860~890840~870850~880Ck351.11810.035≤0.03Cm1.10.00.020>27048021193518035~0.03516~100~670软化退火;正火;调质,应在订货时明确供货状态。如订货时未指定,则以不处理状态供货。6.对Ck、Cm的35~60牌号,可要求淬透性,标准中规定了端淬试验中HRC的界限值,本表略去,对此请参阅标准正文。7.调质状态的力学性能是以经热处理的试样试验而得,对不同的产品规格规定了不同的试样直径。本表中省略,欲了解此项指标请参阅标准正文。8.订货时可经C401.05110.37~0.440.400.50~0.800.045≤0.045≤16320530~7201917197870850~880830~860840~870Ck401.11860.035≤0.03Cm401.11890.0350.020~0.035>16~100290530~7201917C451.05030.42~0.500.400.50~0.800.045≤0.045≤16340580~7701715207850840~870820~850830~860Ck451.11910.035≤0.03Cm451.12010.0350.020~0.035>16~100305580~7701715C501.05400.47~0.550.400.60~0.900.045≤0.045≤16355600~8201614217850835~865810~840820~850Ck501.12060.035≤0.03Cm501.12410.0350.020~0.035>16~100320600~8201614C551.05350.52~0.60.400.60~0.90.045≤0.045≤16370630~8701513229830830~860805~835815~845Ck551.12030.035≤0.03Cm551.1209000.0350.020~0.035>16~100330630~8701513供需双方商定的检验项目有:成品分析(标准中规定了成品分析允许偏差);晶粒度(要求细晶粒则晶粒度应不大于5级);非金属夹杂物(标准中规定了特性指标K值);无损检验;表面脱碳层等。9.用户应在订货时指定材料检验证明书的类别和检验范围。10.本标准现已被DINEN10083-96所代替。C601.06010.57~0.650.400.60~0.900.045≤0.045≤16380650~9201412241830820~850800~830810~840Ck601.12210.035≤0.03Cm601.12230.0350.020~0.035>16~100340650~9201412标准号及牌号材料号化学成分(熔炼分析)%软化退火状态(G)渗碳温度℃淬火温度℃回火温度备注CSi不大MnP不大于SCrMoNi中心淬火(一表面淬火(二次标准名称于布氏硬度不大于次淬火)淬火)℃DIN17210(1986)表面硬化钢供货技术条件C101.03010.007~0.130.400.30~0.600.0045≤0.045---131880~980880~920780~820150~2001.表面硬化钢是含碳量相当低的优质结构钢。表面淬碳或渗氮后淬火硬化可得到高硬度,耐磨的表面层和高韧性芯部的结构件,本表列出仅为非合金钢,还有14个合金结构钢。详见标准。2.表列牌号的其他技术要求和冶炼方法、供货状态、其他技术要求等与DIN17200中的相应牌号相同。3.本标准现已被DINEN10084-98所代替。Ck101.11210.035≤0.035C151.04010.12~0.180.400.30~0.600.045≤0.045---143Ck151.11410.035≤0.035Cm151.11400.0350.020~0.035德国工业标准DIN标准号及标牌号材料号化学成分(熔炼分析)%产品厚度正火状态下的力学性能软化退火状态(G)端淬试验淬火温度软化退火温度℃正火处理淬火温度回火温度备注CSi不MnP不S屈服点抗拉强度最小伸长率,%L0=5.65水淬℃油淬℃准名称大于大于mmRRO.2不小于MPaMPa纵向横向布氏硬度不大于℃℃℃C221.04020.17~0.240.400.30~0.600.045≤0.045≤100230400~5502725156-650~700880~910860~890-540~6801.调质钢是指其化学成分适用于淬硬、在调质状态下具规定的强度同时有良好韧性。表中仅列出非合金钢,本标准还有28个合金钢,详见标准正文。2.牌号中k:含P、S较低的非合金优质钢m:含S带上下限的非合金优质钢。3.冶炼方法由制造厂选择。4.钢必须是镇静钢(不得为半镇静钢)。5.钢板的供货状态可以是:Ck221.11510.035≤0.03Cm221.11490.0350.020~0.035C251.04060.22~0.290.400.40~0.700.045≤0.045≤16260420~5702523156-880~910860~890-Ck251.11580.035≤0.03Cm251.11630.0350.020~0.035>16~100240420~5702523C301.05280.27~0.340.
本文标题:德国工业标准DIN
链接地址:https://www.777doc.com/doc-1085154 .html