您好,欢迎访问三七文档
当前位置:首页 > 建筑/环境 > 工程监理 > 贝克休斯压裂工具介绍
1©2014BakerHughesIncorporated.AllRightsReserved.©2014BAKERHUGHESINCORPORATED.ALLRIGHTSRESERVED.TERMSANDCONDITIONSOFUSE:BYACCEPTINGTHISDOCUMENT,THERECIPIENTAGREESTHATTHEDOCUMENTTOGETHERWITHALLINFORMATIONINCLUDEDTHEREINISTHECONFIDENTIALANDPROPRIETARYPROPERTYOFBAKERHUGHESINCORPORATEDANDINCLUDESVALUABLETRADESECRETSAND/ORPROPRIETARYINFORMATIONOFBAKERHUGHES(COLLECTIVELYINFORMATION).BAKERHUGHESRETAINSALLRIGHTSUNDERCOPYRIGHTLAWSANDTRADESECRETLAWSOFTHEUNITEDSTATESOFAMERICAANDOTHERCOUNTRIES.THERECIPIENTFURTHERAGREESTHATTHEDOCUMENTMAYNOTBEDISTRIBUTED,TRANSMITTED,COPIEDORREPRODUCEDINWHOLEORINPARTBYANYMEANS,ELECTRONIC,MECHANICAL,OROTHERWISE,WITHOUTTHEEXPRESSPRIORWRITTENCONSENTOFBAKERHUGHES,ANDMAYNOTBEUSEDDIRECTLYORINDIRECTLYINANYWAYDETRIMENTALTOBAKERHUGHES’INTEREST.贝克休斯压裂工具和连续油管工具介绍2©2014BakerHughesIncorporated.AllRightsReserved.内容提纲QuickDrill快钻复合桥塞技术全溶解桥塞技术FracPoint™裸眼分段压裂技术OptiPort™无限级固井滑套压裂技术一球开启多个压裂滑套技术重复压裂跨隔封隔器技术贝克休斯套管修复工具过油管工具连续油管工具3©2014BakerHughesIncorporated.AllRightsReserved.一、QUIK-Drill快钻桥塞4©2014BakerHughesIncorporated.AllRightsReserved.桥塞射孔联作E-4SettingToolE-4坐封工具PerfGuns射孔枪CompositePlug复合材料桥塞•固井•多层电缆传输射孔或者TCP射孔•水平井用复合材料桥塞设计5©2014BakerHughesIncorporated.AllRightsReserved.HPHTGen3.0Hi-ValueFastFrac耐温:450F°耐压差:12,500psi耐温:350F°耐压差:10,000psi耐温:275F°耐压差:8,000psi耐温:200F°耐压差:5,000psi易钻桥塞的特性尺寸:2-7/8”to7”6©2014BakerHughesIncorporated.AllRightsReserved.■带生产通道的桥塞:压后可以直接提供试气/生产通道。–投球式–单流阀式■无生产通道桥塞:压裂完成之后需要磨掉才可以进行生产。投球式单流阀式全堵塞式易钻桥塞的特性7©2014BakerHughesIncorporated.AllRightsReserved.与市场普通复合桥塞对比优势性能对比工具材料普通桥塞:金属心轴,钻磨困难贝克桥塞:全部复合材料,易钻(5-10分钟)剪切部件普通桥塞:剪切销钉,钻磨有销钉残余贝克桥塞:剪切环,连接稳固,没有销钉残余密封件普通桥塞:标准/多组胶皮贝克桥塞:叠合胶皮,稳定易钻卡瓦材料普通桥塞:全金属或键式卡瓦贝克桥塞:最少的金属材料,最大化卡瓦咬合BOT’sCompositeSlipsBOT’sSlipInsertCompetitorA’sSlipButtonSlipsCompetitorB’sSlipShearRingShearWasherShearRingShearWasher8©2014BakerHughesIncorporated.AllRightsReserved.8目前可用使用尺寸红色部分为可用于四川区域5.5”26#套管用桥塞4139©2014BakerHughesIncorporated.AllRightsReserved.413复合材料桥塞江汉承压测试报告910©2014BakerHughesIncorporated.AllRightsReserved.下部管柱组成PerfGuns射孔枪E-4SettingTool坐封工具CompositePlug桥塞11©2014BakerHughesIncorporated.AllRightsReserved.复合桥塞下入座封工具1.E-4型电缆座封工具2.用于连续油管或管柱的J型液压座封工具“J”型水力座封工具12©2014BakerHughesIncorporated.AllRightsReserved.其他改进■改造磨鞋适配器使之与20号E-4做封工具能够配套使用■贝克桥塞配套磨鞋,专为磨铣贝克复合桥塞而设计■高扭矩马达,能够在钻磨时提供更高的钻压■金属降阻剂,帮助连续油管下入更深■高粘液体,携带桥塞磨屑■井下干预小组,制定桥塞泵送和磨铣方案,并优化设计■贝克资深现场工程师现场服务■贝克全球技术支持13©2014BakerHughesIncorporated.AllRightsReserved.特殊磨铣工具■贝克研发的新切削矩阵技术■现场应用案例•同一个磨铣工具,在不需要维护情况下完成两口井79个桥塞的钻磨工作•一趟钻完成40个球座钻磨•一趟钻完成48个HV桥塞钻磨•一趟钻完成42个HPHT桥塞钻磨原始镶嵌钻磨43个桥塞后钻磨79个桥塞后14©2014BakerHughesIncorporated.AllRightsReserved.四川地区桥塞钻磨统计■单井一趟钻钻磨所有桥塞,共17个。■BHI磨鞋客户:EOG,Shell,Yilong,Petro-King,Sinopec,Anton,Landy,Jereh,Jianghan,Delta,Zhongyuan井深桥塞数量桥塞下入速度泵送排量泵送压力3300m12ea20-45m/min1-2M315-17Mpa井深钻磨桥塞数量磨鞋下入速度下入排量下入压力钻磨排量钻磨压力钻压平均钻磨时间最快钻磨速度3300m12ea22m/min200L/min17MPa400L/min23-25Mpa1-1.5T30min10min桥塞磨铣案例-克拉玛依Xia92-H15©2014BakerHughesIncorporated.AllRightsReserved.复合压裂桥塞入井统计16©2014BakerHughesIncorporated.AllRightsReserved.近年中国销售使用记录438桥塞:337套(5-1/2”15.5-23#Casing)主要是使用地区:长宁,威远,吉林,江苏,新疆,中原413桥塞:130套(5-1/2”26#Casing)主要使用地区:长宁,威远,作业日期OpsDate作业公司Company目标层位Formation垂深(米)TVD(m)水平段长(米)LateralLength(m)套管尺寸CSGSize桥塞型号PlugSize桥塞数量PlugQTY桥塞平均下入速度PlugDeploymentRate是否成功SuccessornotDecember-14ChangNingLongMaXi2,2582,3425.5''26.8ppf4132242m/minYESDecember-14ChangNingLongMaXi2,9901,5105.5''26.8ppf4131542m/minYESNovember-14SinopecSWQiongZhuSi3,2911,3255.5''23ppf4381460m/minYESJanuary-15ChangNingLongMaXi2,5971,4735.5''26.8ppf4131742m/minYESJanuary-15ChangNingLongMaXi2,5991,4365.5''26.8ppf4131342m/minYESJanuary-15ChangNingLongMaXi3,0001,5005.5''26.8ppf4131742m/minYES17©2014BakerHughesIncorporated.AllRightsReserved.二、SPECTRE™全可溶压裂桥塞18©2014BakerHughesIncorporated.AllRightsReserved.SPECTRE全可溶压裂桥塞业内首个完全可溶的压裂桥塞压裂后无需钻磨直接生产无碎屑残留全通径生产流道19©2014BakerHughesIncorporated.AllRightsReserved.贝克休斯压裂桥塞产品系列对比桥塞类型压裂后无需井筒干预全通径生产通道灵活选择压裂位置FLASH™快钻式复合压裂桥塞SPECTRE™全可溶压裂桥塞20©2014BakerHughesIncorporated.AllRightsReserved.与同行业其他可溶桥塞对比,贝克休斯全可溶桥塞具有以下优势:贝克可溶桥塞全部部件均为可溶材料,包括卡瓦和胶皮,其他同行的产品卡瓦是由陶瓷块或硬质合金块,无法溶解而且硬度比P110套管还要大,容易造成井下硬卡;贝克可溶桥塞材质在滑溜水和压裂液中不溶解,只在返排液中溶解,能保证压裂作业顺利进行,而同行中有的产品在清水中(超过91°C)就会溶解,无法保证压裂能否顺利实施;贝克休斯卡瓦设计为一体式,同行中有的产品为分瓣式,虽然外面有铁丝束缚,但容易产生提前坐封事故。SPECTRE全可溶压裂桥塞优势某公司桥塞产品:陶瓷卡瓦,清水超过91摄氏度会溶解某公司桥塞产品:陶瓷卡瓦,卡瓦分瓣,仅靠束缚带保护,下井时容易提前坐封21©2014BakerHughesIncorporated.AllRightsReserved.主要部件工作原理桥塞本体■与IN-Tallic™可溶球相同材质,控制电解金属(CEM),IN-Tallic™可溶球在全球已应用于超过100,000级压裂,压裂时强度稳定,暴露于返排液后溶解性能优良■溶解速率受盐度和温度影响,可计算预测锚定卡瓦■采用镍基合金涂层技术(0.25mm-0.38mm粒径)■在返排液中溶解成细小碎片,返排出井筒胶皮■材质为贝克休斯研制的特殊聚氨酯材料■暴露在返排液中足够时间后开始溶解,溶解成细小碎片,返排出井筒22©2014BakerHughesIncorporated.AllRightsReserved.01000200030004000500060002hr4hr8hr12hr16hr20hr24hr36hr48hr3day4day5day6day7day8day9dayJ-105材质桥塞本体在长宁返排液中的溶解曲线(100⁰C-105⁰C)胶塞本体重量:5700mg平均溶解速率:21.8mg/cm2/hr溶解时间本体质量(mg)主要部件工作原理桥塞本体23©2014BakerHughesIncorporated.AllRightsReserved.可降解胶皮■在一定温度和盐度的液体环境中一定时间后,胶皮开始降解,形成2.5-28mm不等的不规则碎屑,数量质量不定,随返排返回地面,不影响返排和生产主要部件工作原理24©2014BakerHughesIncorporated.AllRightsReserved.主要部件工作原理可降解卡瓦涂层■在一定温度和盐度的液体环境中一定时间后,镍基合金涂层在返排液环境中逐渐降解剥落,形成6-25mm不等的条状碎屑,数量质量不定
本文标题:贝克休斯压裂工具介绍
链接地址:https://www.777doc.com/doc-4447588 .html