您好,欢迎访问三七文档
当前位置:首页 > 商业/管理/HR > 质量控制/管理 > 高性能混凝土配合比计算公式
体积法计算:制件日期使用部位坍落度含气量α=3.00%Sm=41.00%ρs=2620ρg=2760备注mwmcmp1mp2mams165338850.005.5705.05781000304026300.0010702620Vs.g=0.656W/C:0.39ms=705.058mg=1068.81水泥粉煤灰砂子碎石外加剂水网状纤维33885705.057841068.81045165体积法计算:制件日期使用部位坍落度含气量α=3.00%Sm=40.00%ρs=2620ρg=2760mwmcmp1mp2ma165357890.005.81000304026300.001070W/C:0.37Vs.g=0.648ms=679.424mg=1073.59水泥粉煤灰砂子碎石外加剂水网状纤维体积法计算:制件日期使用部位坍落度含气量α=3.00%Sm=39.00%ρs=2620ρg=2760mwmcmp1mp2ma165377940.006.121000304026300.001070W/C:0.35Vs.g=0.640ms=653.467mg=1076.71C40细石混凝土配合比体积法计算表材料密度(kg/m3)每立方米混凝土材料用量(kg)材料密度(kg/m3)每立方米混凝土材料用量(kg)材料密度(kg/m3)每立方米混凝土材料用量(kg)mg1068.812770项目指标102031.540162031.54010~3019017016015020018517516535~5020018017016021019518517555~7021019018017022010519518575~90215195185175230215205195项目指标10204016204016~2017516014518017015511~151801651501851751605~10185170155190180165表5.2.1-2塑性混凝土的用水量(kg/m3)拌合物稠度卵石最大粒径(mm)碎石最大粒径(mm)维勃稠度(s)坍落度(mm)注:①本表用水量系采用中砂时的取值。采用细砂时,每立方米混凝土用水量可增加5~10kg;采用粗砂时,可减少5~10kg。②掺用矿物掺合料和外加剂时,用水量应相应调整。表5.2.1-1干硬性混凝土的用水量(kg/m3)拌合物稠度卵石最大公称粒径(mm)碎石最大粒径(mm)采用普通硅酸盐水泥时45403530≤0.400.40〉0.40—表3.0.5-1钢筋混凝土中矿物掺合2料最大掺量矿物掺合料种类水胶比最大掺合料(%)采用硅酸盐水泥时粉煤灰粒化高炉矿渣粉钢渣粉硅灰磷渣粉1055≤0.40301065553055452020——≤0.40〉0.40复合掺合料655545注:1采用其他通用硅酸盐水泥时,宜将水泥混合材掺量20%以上的混合材量计入矿物掺合料;2复合材料掺合料各组分得掺量不宜超过单掺时的最大值;3在混合使用俩种或两种以上矿物掺合料时,矿物掺合料总掺量应复合表中复合掺合料的规定。0.60.550.5≤0.45水胶比(W/B)1020401620400.4026~3225~3124~3030~3529~3427~320.5030~3529~3428~3333~3832~3730~350.6033~3832~3731~3636~4135~4033~380.7036~4135~4034~3939~4438~4336~41表3.0.4混凝土的最小胶凝材料用量最大水胶比最小胶凝材料用量(kg/m3)素混凝土钢筋混凝土2.采用人工砂配制混凝土时,砂率可适当增大;250280300280300300预应力混凝土3203303.只用一个单粒级粗骨料配制混凝土时,砂率应适当增大;表5.4.1混凝土的砂率(%)卵石最大公称粒径(mm)碎石最大粒径(mm)4.对薄壁构件,砂率宜取偏大值。1.本表数值系中砂的选用砂率,对细砂或粗砂,可相应地减少或增大砂率;水泥粉煤灰矿粉砂小石中石大石水外加剂50688816299.8749.5449.72705.566试拌15升7.5901.3201.2150.0904.49711.2436.7464.0500.083试件成型40升20.2403.5203.2400.24011.99229.98017.98810.8000.223水泥粉煤灰矿粉砂小石中石大石水外加剂47182757309772.5463.52705.181试拌15升7.0651.2301.1250.1054.63511.5886.9534.0500.078试件成型40升18.8403.2803.0000.28012.36030.90018.54010.8000.207第1组每盘用量第2组每盘用量水泥粉煤灰矿粉砂小石中石大石水外加剂54795886288.8722433.22706.017试拌15升8.2051.4251.3200.0904.33210.8306.4984.0500.090试件成型40升21.8803.8003.5200.24011.55228.88017.32810.8000.241第3组每盘用量α=3.60%Sm=38.00%ρs=2620ρg=2770W/B=0.4水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304026300.00107026202770mwmcmp1mp2mamsmg270.00506.0088.0081.005.566486.74839.62规格项目小石中石大石Vs.g=0.489ms=486.740mg=839.621比例20.00%50.00%30.00%水泥粉煤灰矿粉砂小石中石大石水外加剂纤维506.00088.00081.000486.740167.924419.810251.886270.0005.5661.8试拌15升7.591.321.2157.3012.5196.2973.7784.050.0830.027###########22.773.963.64521.9037.55718.89111.33512.150.250.081制件日期使用部位坍落度含气量实测容重混凝土配合比体积法计算表(一)各原材材料密度(kg/m3)掺合料混凝土含气量(%)质量砂率(%)细骨料表观密度(kg/m3)水胶比计算结果骨料的绝对体积(m3)每立方米混凝土材料用量(kg)粗骨料骨料表观密度(kg/m3)需输入配制参数配合比细骨料用量(kg)粗骨料用量(kg)α=3.60%Sm=39.00%ρs=2620ρg=2770W/B=0.43水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304026300.00107026202770mwmcmp1mp2mamsmg270.00471.0082.0075.005.181514.01850.00规格项目小石中石大石Vs.g=0.503ms=514.011mg=849.995比例20.00%50.00%30.00%水泥粉煤灰矿粉砂小石中石大石水外加剂纤维471.00082.00075.000514.011167.924419.810251.886270.0005.1811.8试拌15升7.0651.231.1257.712.5196.2973.7784.050.0780.027###########18.843.28320.566.71716.79210.07510.80.2070.072制件日期使用部位坍落度含气量实测容重配合比计算结果骨料的绝对体积(m3)细骨料用量(kg)粗骨料用量(kg)C40细石混凝土配合比体积法计算表(二)需输入配制参数混凝土含气量(%)质量砂率(%)细骨料表观密度(kg/m3)水胶比每立方米混凝土材料用量(kg)粗骨料骨料表观密度(kg/m3)各原材材料密度(kg/m3)掺合料α=3.60%Sm=41.00%ρs=2620ρg=2760W/B=水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304026300.00107026202770mwmcmp1mp2mamsmg165.00338.0085.000.005.500698.610.00规格项目小石中石大石Vs.g=0.650ms=698.613mg=1059.040比例20.00%50.00%30.00%水泥粉煤灰矿粉砂小石中石大石水外加剂纤维338.00085.0000.000698.613167.924419.810251.886165.0005.5001.8试拌15升5.071.275010.4792.5196.2973.7782.4750.0830.027###########13.523.4027.9456.71716.79210.0756.60.220.072制件日期使用部位坍落度含气量实测容重粗骨料用量(kg)配合比每立方米混凝土材料用量(kg)计算结果骨料的绝对体积(m3)细骨料用量(kg)需输入配制参数混凝土含气量(%)质量砂率(%)细骨料表观密度(kg/m3)C40细石混凝土配合比体积法计算表(三)水胶比各原材材料密度(kg/m3)掺合料粗骨料骨料表观密度(kg/m3)浆体体积0.323α=2.80%Sm=40.00%ρs=2620ρg=2770W/B=0.397水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304024300.00107026202770mwmcmp1mp2mamsmg1553127805.466709.511125.20规格项目小石中石大石Vs.g=0.677ms=709.510mg=1125.196比例100.00%0.00%0.00%水泥粉煤灰矿粉砂小石中石大石水外加剂纤维3127807101125001555.4661.8试拌15升4.6851.171010.64316.878002.3250.0820.027试件成型45升14.0553.514031.92850.634006.9750.2460.081制件日期使用部位坍落度含气量实测容重配合比计算结果骨料的绝对体积(m3)细骨料用量(kg)粗骨料用量(kg)混凝土配合比体积法计算表(一)需输入配制参数混凝土含气量(%)质量砂率(%)细骨料表观密度(kg/m3)粗骨料骨料表观密度(kg/m3)水胶比各原材材料密度(kg/m3)掺合料每立方米混凝土材料用量(kg)浆体体积0.328α=2.80%Sm=39.00%ρs=2620ρg=2770W/B=0.377水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304026300.00107026202770mwmcmp1mp2mamsmg1553298205.756686.811135.75规格项目小石中石大石Vs.g=0.672ms=686.813mg=1135.749比例100.00%0.00%0.00%水泥粉煤灰矿粉砂小石中石大石水外加剂纤维3298206871136001555.7561.8试拌15升4.9341.233010.30217.036002.3250.0860.027试件成型40升13.1563.289027.47345.43006.20.230.072制件日期使用部位坍落度含气量实测容重C40细石混凝土配合比体积法计算表(二)需输入配制参数混凝土含气量(%)质量砂率(%)每立方米混凝土材料用量(kg)水胶比细骨料表观密度(kg/m3)粗骨料骨料表观密度(kg/m3)各原材材料密度(kg/m3)掺合料计算结果骨料的绝对体积(m3)细骨料用量(kg)粗骨料用量(kg)配合比浆体体积0.314α=2.80%Sm=41.00%ρs=2620ρg=2760W/B=0.417水水泥外加剂细骨料粗骨料ρwρcρp1ρp2ρaρsρg1000304026300.00107026202770mwmcmp1mp2mamsmg1552977405.204736.961117.17规格项目小石中石大石Vs.g=0.686ms=
本文标题:高性能混凝土配合比计算公式
链接地址:https://www.777doc.com/doc-6864134 .html